摘要:The paper presents the results of a study of the microhardness of the WNF-95 sintered electroerosive powder alloy. Powder alloy W-Ni-Fe95 was obtained by electroerosive dispersion of tungsten-containing waste in a kerosene medium. The resulting electroerosive powder alloy W-Ni-Fe 95was pressed in a vacuum chamber and sintered by the method of spark plasma sintering. The aim of this work was to study the microhardness of the WNF-95 sintered powder alloy obtained by the electroerosive dispersion of tungsten-containing waste in a kerosene medium. It has been established that the microhardness of samples sintered by the method of spark plasma sintering from particles of W-Ni-Fe 95alloy dispersed by electric erosion obtained in lighting kerosene is 2185.8 MPa and 2268.0 MPa, indicating their suitability for the manufacture of tungsten-nickel-iron alloys.